What are you looking for?
Products, article numbers, services, inspiration, brochures, ... We will find what you are looking for.
Your target group has been successfully activated.

Would you like to learn more about the benefits you will enjoy?

Learn more
Your target group has been successfully activated.

Would you like to learn more about the benefits you will enjoy?

Learn more
Your target group has been successfully activated.

Would you like to learn more about the benefits you will enjoy?

Learn more
EN/AE

Mirror effect

Turn flat glass and textured glass into mirror glass.

Transform flat glass into mirror surfaces

Hesse PU Mirror lacquer is a light fast PU Effect lacquer for coating onto glass. This fast-drying lacquer material has good adhesion properties and is particularly suitable for striking and creative surface accents on white glass. It acquires an antique effect when a special agent is added to the Mirror lacquer.

Fields of application : in the complete field of interior fittings on white glass within living areas, but also on textured glass.

How to – Mirror effect

  • Object furnishing, textured glass; substrate preparation: Use Cleaning thinner ZD 101 to carefully clean and degrease the textured glass
  • Coating: 1 x 60 - 80 g/m² PU Mirror lacquer DB 46334-M0966, mixing ratio (by volume) 25 : 1 with PU Hardener DR 4076-0002
  • Intermediate drying: 15 - 30 min / 20 °C
  • Use a gauze rag and light pressure to clean any spray mist from surfaces
  • Top coat: 1 x 100 - 120 g/m² UNA-COLOR Glass colour lacquer DB 42105-1013, mixing ratio (by volume) 5 : 1 with PU Hardener DR 4076-0001 and addition of 5 – 10 % Thinner DV 4900 to the lacquer/ hardener mixture.
  • Packable: after drying for at least 16 h / 20 °C
  • Ready for assembly or gluing: after 5 d / 20 °C
  • Glass partition wall with Antique effect
  • Surface preparation: Use Cleaning thinner ZD 101 to carefully clean and degrease the glass
  • Effect creation: Spray Effect agent DZ 4992-05856 thinly onto the edges of the glass surface.
  • After brief intermediate drying, use moistened greaseproof paper to dab on the desired effect.
  • Then coat with 60 - 80 g/m² PU Mirror lacquer DB 46334-M0966, mixing ratio (by volume) 25 : 1 with PU Hardener DR 4076-0002.
  • Intermediate drying: 15 - 30 min / 20 °C
  • Use a gauze rag and light pressure to clean any spray mist from surfaces
  • Top coat: 1 x 100 - 120 g/m² UNA-COLOR Glass colour lacquer DB 42105-8004, mixing ratio (by volume) 5 : 1 with PU Hardener DR 4076-0001 and addition of 5 – 10 % Thinner DV 4900 to the lacquer/ hardener mixture.
  • Packable: after at least 16 h / 20 °C
  • Ready for assembly and/or gluing after 5 d / 20 °C

Products required

PU Mirror lacquer
DB 46334-M0966
UNA-COLOR Glass colour lacquer
DB 42105-1013
Effect agent
DZ 4992-05856
Interested in a sample?
Obtain additional inspiration

You’ll find more effects in our Sample shop. Make your choice and order your desired sample free of charge.

Processing and safety information
Please observe the latest technical information and the material safety data sheets for the stated individual products. Please conduct a test coating under real conditions. Please follow the precise specifications for addition of hardeners and thinners and the drying times included in the effect creation information set out below. Ensure careful stirring or respectively mixing in of all necessary components.
 
Note
This information is purely advisory and is based on the best knowledge available after careful research in line with current state of the art technology. It is not legally binding. We also refer you to our Terms and Conditions. The material safety data sheet as per regulation (EC) No. 1907/2006 is available.